Texin? 250

Texin? 250

Manufacturer: Covestro
Produced At:
 Europe / China
Product Category: TPU
Product No: Texin 250 
Product Quantity: 25KG / BAG
Product Features: Abrasion Resistant,Chemical Resistant,Low Gel,Medium Clarity,Oil Resistant,Solvent Resistant

Texin? 250

Thermoplastic Polyurethane Elastomer (Polyester)
Product Description:

Texin 250 resin is an aromatic polyester-based thermoplastic polyurethane with a Shore hardness of approximately 50D. It is processed primarily by extrusion and blow molding but can also be used for injection molding.


Features 
  • Abrasion Resistant,Chemical Resistant,Low Gel,Medium Clarity,Oil Resistant,Solvent Resistant
Uses 
  • Film,Footwear,Hose,Profiles,Sheet,Tubing
Agency Ratings 
  • FDA 21 CFR 177.1680,FDA 21 CFR 177.2600 
Appearance 
  • Natural Color

Processing Method 
  • Blow Molding,Extrusion,Injection Molding
Physical
Nominal Value
Unit
Test Method
Density / Specific Gravity



--
1.22

ASTM D792
--
1.22
g/cm3
ISO 1183
Molding Shrinkage



Flow : 0.100 in
8.0E-3
in/in
ASTM D955
Across Flow : 0.100 in
8.0E-3
in/in
ASTM D955
Across Flow : 0.100 in
0.80
%
ISO 2577
Flow : 0.100 in
0.80
%
ISO 2577
Hardness
Nominal Value
Unit
Test Method
Durometer Hardness


ASTM D2240, ISO 868
Shore A
95


Shore D
50


Mechanical
Nominal Value
Unit
Test Method
Flexural Modulus


ASTM D790, ISO 178
73°F
12000
psi

158°F
5220
psi

Taber Abrasion Resistance



1000 Cycles, 1000 g, H-18 Wheel
70.0
mg
ASTM D1044
1000 Cycles, 1000 g, H-18 Wheel
70.0
mg
ISO 4649
Elastomers
Nominal Value
Unit
Test Method
Tensile Stress


ASTM D412, ISO 37
100% Strain
1700
psi

300% Strain
4600
psi

Tensile Strength (Yield)
6700
psi
ASTM D412, ISO 37
Tensile Elongation (Break)
400
%
ASTM D412, ISO 37
Tear Strength



-- 2
775
lbf/in
ASTM D624
--
780
lbf/in
ISO 34-1
Compression Set 3


ASTM D395B, ISO 815
73°F, 22 hr
15
%

158°F, 22 hr
35
%

Bayshore Resilience
25
%
ASTM D2632
Thermal
Nominal Value
Unit
Test Method
Glass Transition Temperature
-4.00
°F
DMA
Vicat Softening Temperature
239
°F
ISO 306/A50, ASTM D1525 4
Injection
Nominal Value
Unit

Drying Temperature - Desiccant Dryer
199 to 219
°F

Drying Time - Desiccant Dryer
2.0
hr

Suggested Max Moisture
0.030
%

Suggested Max Regrind
20
%

Rear Temperature
374 to 410
°F

Middle Temperature
374 to 419
°F

Front Temperature
392 to 428
°F

Nozzle Temperature
401 to 437
°F

Processing (Melt) Temp
401 to 419
°F

Mold Temperature
59 to 104
°F

Injection Pressure
6000 to 15000
psi

Injection Rate
Slow-Moderate


Back Pressure
< 200
psi

Screw Speed
40 to 80
rpm

Cushion
0.125
in

Injection Notes
Hold Pressure: 60 to 80% of Injection Pressure
Extrusion
Nominal Value
Unit

Drying Temperature
199 to 219
°F

Drying Time
2.0
hr

Suggested Max Regrind
20
%

Cylinder Zone 1 Temp.
356 to 392
°F

Cylinder Zone 3 Temp.
356 to 401
°F

Cylinder Zone 5 Temp.
356 to 410
°F

Melt Temperature
374 to 401
°F

Die Temperature
365 to 410
°F



Products are widely used in plastic modification, automotive, construction, electrical and electronic, industrial, daily necessities and other fields


Consultation
展開
主站蜘蛛池模板: 欧美成人精品高清视频在线观看 | 色老板精品视频在线观看| 日本熟妇乱人伦a片免费高清| 国产精品亚洲а∨天堂123| 无码熟妇αⅴ人妻又粗又大| 成人国产一区二区日韩| 成人一区二区三区视频在线观看 | 特级西西人体444www高清大胆| 欧美丰满熟妇乱xxxxx视频| 亚洲熟妇无码乱子av电影| 久久婷婷五月综合色和啪| 精产国品一二三产品蜜桃| 亚洲国产老鸭窝一区二区三区| 久久精品aⅴ无码中文字字幕| 男男啪啪激烈高潮cc漫画免费 | 狠狠躁夜夜人人爽天96| 国产内射xxxxx在线| 末成年女a∨片一区二区| 国产午夜福利100集发布| 日韩国产人妻一区二区三区| 蜜桃av久久久一区二区三区麻豆| 国产免费无遮挡吸奶头视频| 人妻天天爽夜夜爽精品视频| 柠檬福利精品视频导航| 特级国产午夜理论不卡| 久久久久性视频| 曰本女人与公拘交酡| 无码人妻丰满熟妇a片护士| 男女猛烈xx00免费视频试看| 日本肉体xxxx裸体137大胆| 中国极品少妇videossexhd| 久久精品国产精油按摩| 午夜精品一区二区三区免费视频| 国产亚洲欧美另类一区二区三区| 日韩乱码人妻无码中文字幕 | 国产视频播放| 极品尤物被啪到呻吟喷水| 99久久久国产精品免费牛牛| 国产女精品视频网站免费| 免费播放一区二区三区| 久青草久青草高清在线播放|